methanol
p-tert-butoxystyrene
isobornyl acrylate
2,2′-azobis(methyl 2-methylpropionate)
→
p-tert-butoxystyrene isobornyl acrylate
反应条件
详细条件
See reaction.notes.procedure_details.
后处理
- 1温度After cooling
- 2其他to precipitate out
- 3过滤Crystal was recovered by filtration
- 4其他dried under reduced pressure
实验过程
To 70 g (0.397 mole) of p-tert-butoxystyrene and 35.4 g (0.170 mole) of isobornyl acrylate was added 1.5 g of 2,2′-azobis(methyl 2-methylpropionate), followed by conducting a polymerization reaction in 1,4-dioxane under nitrogen gas streams at 80° C. for 6 hours. After cooling, the reaction solution was poured into 5000 ml of aqueous methanol solution to precipitate out. Crystal was recovered by filtration and dried under reduced pressure to give 102.2 g of poly(p-tert-butoxystyrene/isobornyl acrylate) as white powdery crystal. A weight-average molecular weight was found about 56000 by GPC measurement using polystyrene as a standard.