Реакция #438707

ord-ee6f125aac904e21a82a287e76f823af

Уравнение реакции

O=[Si]([O-])[O-].[Na+].[Na+]
water glass
[Na+].[OH-]
sodium hydroxide
[Na+].[Na+].[Na+].[Na+].[O-][Si]([O-])([O-])[O-]
sodium silicate

Реагенты

Нет

Условия реакции

Подробные условия
See reaction.notes.procedure_details.

Обработка

  1. 1
    Другоеspray-dried in a spray tower from Kestner

Методика

(Comparison) 1600 kg of water glass with an SiO2/Na2O ratio of 2.06 and an active substance content of 45.5% were admixed with 36.8 kg of sodium hydroxide solution (48% strength) and spray-dried in a spray tower from Kestner to give an amorphous sodium silicate having an active substance content of 83%. 15 kg of the amorphous sodium silicate are heat-treated at 720° C. for 90 min in a muffle furnace (Nabertherm, model W1000/H). A second batch is treated identically. The chilled materials (about 24 kg) are pulverized using a jaw crusher and a disk mill.

Источник

DOI: 10.6084/m9.figshare.5104873.v1Патент: US06743766B1uspto-grants-2004_06