Реакция #334897
ord-83e27cce764c40d789da328866ec9e7a
Уравнение реакции
Реактанты
Реагенты
Условия реакции
Температура
175°CELSIUS
Подробные условия
See reaction.notes.procedure_details.
Методика
A 10:1 mole ratio of ethylene carbonate to polyester polyol (poly(caprolactone) diol, MW=530) is heated with stirring under a nitrogen atmosphere for 4 hours at 175° C. using 0.5 percent sodium stannate trihydrate as catalyst to give 97.9 percent ethylene carbonate conversion to a poly(alkylene carbonate) polyol with 19.2 percent carbon dioxide. The catalyst is removed as in Example 1.