반응 #987822

ord-f1beee3ba558418d97e68d0687ba65d3

반응 조건

상세 조건
See reaction.notes.procedure_details.

후처리

  1. 1
    기타The prepared solution was reacted at 66° C. for 8 hours
  2. 2
    기타After the reaction
  3. 3
    기타the resulting mixture was precipitated in ethyl ether
  4. 4
    여과filtered
  5. 5
    기타dried under vacuum condition

실험 절차

To 50 g of PGMEA were added 6 g of 9-anthracenemethyl methacrylate, 3 g of t-butylacrylate, 1 g of acrylic acid and 0.8 g of AIBN. The prepared solution was reacted at 66° C. for 8 hours. After the reaction, the resulting mixture was precipitated in ethyl ether, filtered, and dried under vacuum condition thereby obtaining poly(9-anthracenemethyl methacrylate/t-butylacrylate/acrylic acid) having a molecular weight of 11,200 (yield: 80%) (see the NMR spectrum of FIG. 2).

출처

DOI: 10.6084/m9.figshare.5104873.v1특허: US07361447B2uspto-grants-2008_04