  1. 1
    기타The bottle was sealed
  2. 2
    온도The bottle was then heated at 50 degrees Centigrade in a water bath for 18 hours
  3. 3
    기타The bottle was then removed from the water bath
  4. 4
    기타the polymer isolated by extraction with methanol
  5. 5
    기타to precipitate polymer
  6. 6
    기타The polymer was then dried under vacuum

실험 절차

The copolymer of allyl methacrylate and methacrylate was prepared by placing 5 grams of allyl methacrylate, 95 grams of methyl methacrylate, 300 milliliters of methylene chloride, and 1.0 gram of isopropyl peroxydicarbonate in a 28 ounce round bottle. The bottle was sealed. The bottle was then heated at 50 degrees Centigrade in a water bath for 18 hours. The bottle was then removed from the water bath, and the polymer isolated by extraction with methanol to precipitate polymer. The polymer was then dried under vacuum. Thereafter, the molecular weight was determined by inherent viscosity in methylene chloride versus poly(methyl methacrylate), and was found to be in excess of 500,000.

출처

DOI: 10.6084/m9.figshare.5104873.v1특허: US04346197uspto-grants-1982_08