반응 #415503
ord-1d5b085b08a94e0a9c8ead41550eb4ff
반응 조건
상세 조건
See reaction.notes.procedure_details.
후처리
- 1workup.ADDITIONby adding 0.42 ml
- 2기타at room temperature
- 3기타to polymerize for 2 hours
- 4기타yielding 27.5 g
실험 절차
An AB block polymer of styrene-isoprene was prepared by adding 0.42 ml. of 1.18 N sec-butyl lithium to a mixture of 10 g. styrene of 175 ml. of benzene and 5 ml. of tetrahydrofuran at room temperature. The mixture was allowed to polymerize for 2 hours and 40 g. of dry air-free isoprene was added and the polymerization continued for 2 additional hours. The product was isolated by precipitation into methanol, yielding 27.5 g. of block polymer dispersant.