  1. 1
    workup.ADDITIONmixed with 1,000 g

실험 절차

50 Grams of N,N-diethylaminoethyl methacrylate, 50 g. of methyl methacrylate, 1 g. of Dupanol ME, 1 g. of Emulphor ON-870, 6 g. of ethylene diacrylate, 1 g. of potassium persulfate, and 0.5 g. of sodium bisulfite are dissolved or mixed with 1,000 g. of water. This mixture is tumbled in a water bath at 60° C. for 24 hr. to obtain a crosslinked copolymer of methyl methacrylate and N,N-diethylaminoethyl acrylate. The crosslinked polymer is separated from the aqueous dispersion by the method described in Example 4.

출처

DOI: 10.6084/m9.figshare.5104873.v1특허: US04177255uspto-grants-1979_12