반응 #1379901

ord-f7b914a1905a4d9e9f10b720b5dd5864

반응 방정식

CCCCCCCCCCC1CC2C=CC1C2
5-decyl-2-norbornene
CC=C1CC2C=CC1C2
5-ethylidene-2-norbornene
CCCCCCC1CC2C=CC1C2
5-hexyl-2-norbornene
CC=C1CC2C=CC1C2.CCCCCCC1CC2C=CC1C2
HNB ENB
C1=CC2CCC1C2
norbornene

반응 조건

상세 조건
See reaction.notes.procedure_details.

후처리

  1. 1
    기타Polymerization
  2. 2
    workup.ADDITIONwere added

실험 절차

Polymerization was conducted in the same manner as in Preparation Example 1 except that 18 parts of 5-hexyl-2-norbornene (HNB) was used in place of 26 parts of 5-decyl-2-norbornene, and 3 parts of 5-ethylidene-2-norbornene (ENB) were added, thereby obtaining 21 parts of a norbornene terpolymer [Mn=71,100, Mw=107,000; compositional ratio NB/HNB/ENB of monomers=74/23/3 (molar ratio); Tg=323° C.] was obtained.

출처

DOI: 10.6084/m9.figshare.5104873.v1특허: US07238405B2uspto-grants-2007_07