반응 #1188
ord-daa2e4e30ef942c09a4a540a3956b1ac
반응 방정식
ethyl acetate
ammonium hydroxide
→
vinyl acetate
vinyl alcohol
용매
반응 조건
상세 조건
See reaction.notes.procedure_details.
후처리
- 1workup.DISSOLUTIONthe polymer dissolved
- 2기타to give a gel
- 3기타During the next three weeks
- 4기타at room temperature
- 5온도At this time the solution was heated
- 6기타to remove ammonia
실험 절차
To 100 g of the same copolymer was added 1500 ml of ethyl acetate, 40 ml of concentrated ammonium hydroxide and 40 ml of water. After two days with stirring, the polymer dissolved to give a gel. During the next three weeks at room temperature, a progressive decrease in viscosity of the solution was noted. At this time the solution was heated to remove ammonia, giving a partially saponified polymer of composition 32.4 wt % vinyl acetate, 16.4 wt % vinyl alcohol, 38 wt % TFE, and 13.2 wt % HFP in a 27.4 wt % solids solution in ethyl acetate.