反応 #987822
ord-f1beee3ba558418d97e68d0687ba65d3
反応方程式
PGMEA
methacrylate
t-butylacrylate
acrylic acid
AIBN
→
methacrylate t-butylacrylate acrylic acid
収率 80.0%
反応条件
詳細条件
See reaction.notes.procedure_details.
後処理
- 1その他The prepared solution was reacted at 66° C. for 8 hours
- 2その他After the reaction
- 3その他the resulting mixture was precipitated in ethyl ether
- 4ろ過filtered
- 5その他dried under vacuum condition
実験手順
To 50 g of PGMEA were added 6 g of 9-anthracenemethyl methacrylate, 3 g of t-butylacrylate, 1 g of acrylic acid and 0.8 g of AIBN. The prepared solution was reacted at 66° C. for 8 hours. After the reaction, the resulting mixture was precipitated in ethyl ether, filtered, and dried under vacuum condition thereby obtaining poly(9-anthracenemethyl methacrylate/t-butylacrylate/acrylic acid) having a molecular weight of 11,200 (yield: 80%) (see the NMR spectrum of FIG. 2).