反応 #987821

ord-dbce1ccd94724d1d8199b816cd9170d4

反応条件

詳細条件
See reaction.notes.procedure_details.

後処理

  1. 1
    その他The prepared solution was reacted at 66° C. for 8 hours
  2. 2
    その他After the reaction
  3. 3
    その他the resulting mixture was precipitated in ethyl ether
  4. 4
    ろ過filtered
  5. 5
    その他dried under vacuum condition

実験手順

To 50 g of propylene glycol methyl ether acetate (PGMEA) were added 5 g of 9-anthracenemethyl methacrylate, 1 g of 2-hydroxyethyl methacrylate, 3 g of t-butylacrylate, 1 g of acrylic acid and 0.4 g of AIBN. The prepared solution was reacted at 66° C. for 8 hours. After the reaction, the resulting mixture was precipitated in ethyl ether, filtered, and dried under vacuum condition, thereby obtaining poly(9-anthracenemethyl methacrylate/2-hydroxyethyl methacrylate/t-butylacrylate/acrylic acid) having a molecular weight of 12,500 (yield: 88%) (see the NMR spectrum of FIG. 1).

出典

DOI: 10.6084/m9.figshare.5104873.v1特許: US07361447B2uspto-grants-2008_04