反応 #89802

ord-64150bcd57e847049c37bcfb81e28339

反応条件

詳細条件
See reaction.notes.procedure_details.

後処理

  1. 1
    workup.ADDITIONThe beaker containing the aqueous catalyst solution
  2. 2
    その他is placed in a 50° C.
  3. 3
    その他for 12 hours

実験手順

Robinin/silver colloidal nanoparticle catalyst is prepared by dissolving 1.07 g robinin in a beaker containing 800 ml DI water at room temperature. 1 N NaOH solution is added with stirring to adjust the solution pH to 11. In a separate beaker, 1.42 g silver p-toluenesulfonate is dissolved in 40 ml DI water. The silver ion solution is added to the robinin solution with vigorous stirring. The molar ratio of silver metal to robinin is 1:0.28. The beaker containing the aqueous catalyst solution is placed in a 50° C. water bath for 12 hours to test its stability. After 12 hours the solution is observed and no precipitate is expected indicating that the catalyst is still stable.

出典

DOI: 10.6084/m9.figshare.5104873.v1特許: US09441300B2uspto-grants-2016_09