- 1workup.ADDITIONmixed while boron trifluoride phenol complex
- 2workup.ADDITIONwas slowly added
- 3温度the material was then cooled under dry ice
- 4workup.ADDITIONNext, alkali was added to inactivate and
- 5その他remove the catalyst
- 6濃縮concentrated
- 7その他to remove the solvent and unreacted monomer
実験手順
250 g α-methyl styrene (99.8% purity), 250 g isopropenyltoluene, and 500 g toluene were introduced into a three-mouthed flask, and mixed while boron trifluoride phenol complex was slowly added, and the material was then cooled under dry ice and acetone solvent and reacted for 3 hr at 20° C. Next, alkali was added to inactivate and remove the catalyst, and concentrated to remove the solvent and unreacted monomer, and α-methylstyrene-isopropenyltoluene copolymer was obtained as a residue. This polymer was designated Polymer B3, and its physical properties are listed in Table 2.