反応 #578433

ord-56c73c674f6e45feb107ca90d3d30919

反応条件

温度
67°CELSIUS
詳細条件
See reaction.notes.procedure_details.

後処理

  1. 1
    その他The mixture was polymerized
  2. 2
    その他After completion of the polymerization
  3. 3
    その他the polymerization product was precipitated in n-hexane
  4. 4
    ろ過filtered
  5. 5
    その他dried in vacuo

実験手順

3 g of 4-bromostyrene, 4 g of acrolein, 3 g of methacrylate and 0.2 g of AIBN were sufficiently mixed with 50 g of PGMEA. The mixture was polymerized by heating the mixture at 67° C. for 8 hours. After completion of the polymerization, the polymerization product was precipitated in n-hexane, filtered, and dried in vacuo to give a poly(bromostyrene-acrolein-methacrylate) copolymer.

出典

DOI: 10.6084/m9.figshare.5104873.v1特許: US07531297B2uspto-grants-2009_05