反応 #56354
ord-35eb3f27865c494eb6a02a5dc4b3fcd8
反応方程式
反応条件
詳細条件
See reaction.notes.procedure_details.
後処理
- 1洗浄Coagulated polymer was washed
- 2workup.DISSOLUTIONtwice dissolved in acetone
- 3その他reprecipitated in water in a blender
- 4その他air-dried
- 5その他vacuum-oven dried 3.5 hrs
- 6その他at 72° C., and finally mill-dried at about 130° C
- 7その他The terpolymer produced
実験手順
Coagulated polymer was washed by chopping in a blender with water, twice dissolved in acetone and reprecipitated in water in a blender, then air-dried, vacuum-oven dried 3.5 hrs. at 72° C., and finally mill-dried at about 130° C. Yield: 254 g. The terpolymer produced had an inherent viscosity (chloroform, 30° C.) of 1.51 deciliters/gram and an acid content of 0.24 meq./gram (titration with aqueous sodium hydroxide), or 0.23 meq./gram (titration with alcoholic potassium hydroxide). The terpolymer had 3.3 percent monoethyl fumarate; the remainder was believed to be about equally divided between ethyl acrylate and butyl acrylate.