反応 #1985935

ord-a7bb598f3656488aaec456d3cdfecd9e

溶媒

反応条件

詳細条件
See reaction.notes.procedure_details.

後処理

  1. 1
    温度with warming
  2. 2
    温度to cool

実験手順

Sulfanilic acid (43 g) was dissolved in 2 L of water with warming. The solution was mixed with 200 g of a carbon black having a surface area of 230 m2 /g and a DBPA of 70 ml/100 g and allowed to cool. An aqueous solution of 20.5 g NaNO2 was added slowly and the resulting dispersion was stirred for one hour. 4-Sulfobenzenediazonium hydroxide inner salt was formed in situ, which reacted with the carbon black. The dispersion was filtered through a Whatman #41 filter, and the product was dried in an oven at 70° C. The product has attached p--C6H4SO3- groups.

出典

DOI: 10.6084/m9.figshare.5104873.v1特許: US05571311uspto-grants-1996_11