C=CC(=O)OCCC[SiH2]O[Si](C)(C)C
(3-acryloxypropyl)trimethylsiloxy silane
CC(=O)OC=Cc1ccccc1
acetoxystyrene
CC(C)(C#N)N=NC(C)(C)C#N
AIBN
C=CC(=O)OCCC[SiH2]O[Si](C)(C)C.OC=Cc1ccccc1
hydroxystyrene (3-acryloxypropyl)trimethylsiloxy silane

溶媒

反応条件

温度
65°CELSIUS
詳細条件
See reaction.notes.procedure_details.

後処理

  1. 1
    workup.ADDITIONcharged into a 3-neck flask
  2. 2
    その他The system was then purged with N2 for 30 mins before the temperature
  3. 3
    workup.ADDITIONOn the second day, 100 g methanol and 30 mL 30% ammonia hydroxide were added to the system
  4. 4
    その他was kept at 60° C
  5. 5
    workup.WAITThe reaction was carried out overnight under N2
  6. 6
    その他On the third day, the solution was precipitated in 2000 mL water
  7. 7
    その他The polymer was collected
  8. 8
    その他dried in vacuum oven overnight at 40° C

実験手順

5 g (3-acryloxypropyl)trimethylsiloxy silane, 38 g acetoxystyrene and 2.41 g AIBN were dissolved in 128 g THF and charged into a 3-neck flask. The system was then purged with N2 for 30 mins before the temperature was raised to 65° C. The reaction was carried out overnight under N2. On the second day, 100 g methanol and 30 mL 30% ammonia hydroxide were added to the system and the temperature was kept at 60° C. The reaction was carried out overnight under N2. On the third day, the solution was precipitated in 2000 mL water and 20 mL acetic acid. The polymer was collected and dried in vacuum oven overnight at 40° C. The molecular weight was determined by gel permeation chromatography (GPC) to be 7.5K.

出典

DOI: 10.6084/m9.figshare.5104873.v1特許: US06586156B2uspto-grants-2003_07