Réaction #2354

ord-32f23f9ca43c4245993689b694a4b02b

Réactifs

Aucun

Conditions de réaction

Conditions détaillées
See reaction.notes.procedure_details.

Traitement

  1. 1
    AutreThe copolymer was dried under vacuum (0.1mm Hg) at 110° C. for about 16 hours
  2. 2
    Autreto remove any unreacted monomer
  3. 3
    Autreat 25° C
  4. 4
    Autreat room temperature

Mode opératoire

The procedure in Example 1 was substantially repeated, except that 13.6 mL of 1-dodecanol instead of 4.00 mL of glycerol and 0.12 mL (40 μmol) instead of 0.10 mL of stannous octoate solution were used. The copolymer was dried under vacuum (0.1mm Hg) at 110° C. for about 16 hours to remove any unreacted monomer. The copolymer had an inherent viscosity of 0.15 dL/g in HFIP at 25° C. The copolymer was viscous liquid at room temperature. The molar ratio of PC.L/PLA was found to be 51.5/48.5 by proton NMR.

Source

DOI: 10.6084/m9.figshare.5104873.v1Brevet: US05728752uspto-grants-1998_03