Réaction #1188
ord-daa2e4e30ef942c09a4a540a3956b1ac
Équation de réaction
Réactifs
Aucun
Solvants
Conditions de réaction
Conditions détaillées
See reaction.notes.procedure_details.
Traitement
- 1workup.DISSOLUTIONthe polymer dissolved
- 2Autreto give a gel
- 3AutreDuring the next three weeks
- 4Autreat room temperature
- 5TempératureAt this time the solution was heated
- 6Autreto remove ammonia
Mode opératoire
To 100 g of the same copolymer was added 1500 ml of ethyl acetate, 40 ml of concentrated ammonium hydroxide and 40 ml of water. After two days with stirring, the polymer dissolved to give a gel. During the next three weeks at room temperature, a progressive decrease in viscosity of the solution was noted. At this time the solution was heated to remove ammonia, giving a partially saponified polymer of composition 32.4 wt % vinyl acetate, 16.4 wt % vinyl alcohol, 38 wt % TFE, and 13.2 wt % HFP in a 27.4 wt % solids solution in ethyl acetate.