Réaction #1106652
ord-4b81e6e0b95a4924bcf721e96630daee
Équation de réaction
vinylpyrrolidone
acrylic acid
azobisisobutyronitrile
→
acrylic acid vinylpyrrolidone
Réactifs
Aucun
Conditions de réaction
Conditions détaillées
See reaction.notes.procedure_details.
Traitement
- 1Autrereacted at 80° C. for 9 hours
- 2Autreto polymerize monomers
- 3AutreThe polymerization product was purified by precipitation from hexane
Mode opératoire
58.5 g of vinylpyrrolidone (P-6-1), 70.5 g of acrylic acid (P-6-2), and 9.0 g azobisisobutyronitrile were dissolved in propylene glycol monomethyl ether and reacted at 80° C. for 9 hours to polymerize monomers. The polymerization product was purified by precipitation from hexane to obtain 110 g of a poly(acrylic acid/vinylpyrrolidone) copolymer with an Mw of 5,600 and Mw/Mn of 1.62. This copolymer is indicated as a resin P-6.