Reacción #2354
ord-32f23f9ca43c4245993689b694a4b02b
Ecuación de reacción
Reactantes
Reactivos
Ninguno
Condiciones de reacción
Condiciones detalladas
See reaction.notes.procedure_details.
Tratamiento posterior
- 1OtroThe copolymer was dried under vacuum (0.1mm Hg) at 110° C. for about 16 hours
- 2Otroto remove any unreacted monomer
- 3Otroat 25° C
- 4Otroat room temperature
Procedimiento
The procedure in Example 1 was substantially repeated, except that 13.6 mL of 1-dodecanol instead of 4.00 mL of glycerol and 0.12 mL (40 μmol) instead of 0.10 mL of stannous octoate solution were used. The copolymer was dried under vacuum (0.1mm Hg) at 110° C. for about 16 hours to remove any unreacted monomer. The copolymer had an inherent viscosity of 0.15 dL/g in HFIP at 25° C. The copolymer was viscous liquid at room temperature. The molar ratio of PC.L/PLA was found to be 51.5/48.5 by proton NMR.