Reaction #1880948
ord-2b589cc700b3411e8ab9872cb5abea2f
Reaction equation
Reagents
None
Conditions
Temperature
52.5°CELSIUS
Detailed conditions
See reaction.notes.procedure_details.
Workup
- 1OtherThe resultant reaction mixture
- 2Otherthe upper layer was removed by decantation
- 3OtherThe viscous resinous substance obtained
- 4OtherThe rubbery resin precipitated
- 5Otherwas dried under vacuum
Procedure
In 100 mL of acetone were dissolved 16.2 g of poly(p-hydroxystyrene) and isopropyl chloride. To this reaction mixture was added 1.8 g of triethylamine. This mixture was stirred at 50 to 55° C. for 5 hours. The resultant reaction mixture was transferred to 1,000 mL of water, and the upper layer was removed by decantation. The viscous resinous substance obtained was dissolved in 75 mL of acetone, and this solution was transferred to 500 mL of water. The rubbery resin precipitated was dried under vacuum. Thus, 15.4 g of poly(p-hydroxystyrene/p-isopropoxystyrene) was obtained as a white powder.