Reaktion #468381

ord-25db3c0976104457a5855e41a877733b

Reaktionsgleichung

CC1(C)CC(N=C=O)CC(C)(CN=C=O)C1
isophorone diisocyanate
CCCCCCCCCCCC(=O)[O-].CCCCCCCCCCCC(=O)[O-].CCC[CH2][Sn+2][CH2]CCC
di-n-butyltin dilaurate
C=CC(=O)OCCO
2-hydroxyethyl acrylate
COc1ccc(O)cc1
hydroquinone monomethylether
C=CC(=O)O.C=CC(=O)O.CCOC(N)=O
urethane diacrylate

Lösungsmittel

Reaktionsbedingungen

Temperatur
55°CELSIUS
Detaillierte Bedingungen
See reaction.notes.procedure_details.

Aufarbeitung

  1. 1
    SonstigeInto a 1-liter 3-necked flask provided with a stirrer
  2. 2
    workup.ADDITIONadding dropwise
  3. 3
    workup.ADDITIONAfter completion of the dropwise addition
  4. 4
    Sonstigewas reduced to 60° C.
  5. 5
    TemperaturSince the viscosity increased
  6. 6
    workup.WAITthe reaction was continued for 5 hours at 70° C.

Vorschrift

Into a 1-liter 3-necked flask provided with a stirrer and thermometer were metered in 425 parts of dodecabutyleneglycol (tradename: PTG-850, manufactured by Hodogaya Chemical Industries Co., Ltd, molecular weight 850), 0.43 parts of di-n-butyltin dilaurate, 0.4 parts of hydroquinone monomethylether, followed by stirring at 55° C. and adding dropwise, 222 parts of isophorone diisocyanate in 3 hours. After completion of the dropwise addition, the reaction was further continued for 3 hours at 70° C. and then temperature was reduced to 60° C., then 122 parts of 2-hydroxyethyl acrylate was added dropwise in 2 hours. Since the viscosity increased, 193 parts of n-butyl acetate was added and the reaction was continued for 5 hours at 70° C. to give an urethane diacrylate (UPA-2) with a solids concentration of 80% by weight.

Quelle

DOI: 10.6084/m9.figshare.5104873.v1Patent: US06306502B1uspto-grants-2001_10