- 1SonstigeThe copolymer was dried under vacuum (0.1 mm Hg) at 80° C. for about 80 hours
- 2Sonstigeto remove any unreacted monomer
- 3Sonstigeat 25° C
- 4Sonstigeat room temperature
Vorschrift
The procedure in Example 5A was substantially repeated, except that 68.48 grams (0.60 mole) of ε-caprolactone and 40.83 grams (0.40 mole) of p-dioxanone were used. The copolymer was dried under vacuum (0.1 mm Hg) at 80° C. for about 80 hours to remove any unreacted monomer. The copolymer had an inherent viscosity of 0.19 dL/g in HFIP at 25° C. The copolymer was a liquid at room temperature. The molar ratio of PCL/PDS was found to be 57.2/42.8 by proton NMR.