An undercoating material was prepared as follows. A mixture of 20 parts gamma-methacryloxypropyltrimethoxysilane, 80 parts methyl methacrylate, 100 parts xylene, and 1.0 part azobisisobutyronitrile was mixed and then heated at 100° C. for 3 hours to give gamma-methacryloxypropyltrimethoxysilane-methyl methacrylate copolymer. Xylene was added to this copolymer to prepare an undercoating material having 40 percent solids and a viscosity of 150 cP.