تفاعل #1726659
ord-71f79e01b3bc488cb224515ccfa47cbc
معادلة التفاعل
sodium hydroxide
zirconium oxychloride octahydrate
ammonium chloride
phosphoric acid
→
zirconium phosphate
الكواشف
لا شيء
المذيبات
ظروف التفاعل
الظروف التفصيلية
See reaction.notes.procedure_details.
المعالجة
- 1أخرىthe resulting precipitates
- 2غسيلwere washed well
- 3أخرىcalcined at 900° C
- 4أخرىobtained by the calcination
الإجراء التجريبي
0.2 mol of zirconium oxychloride octahydrate and 0.05 mol of ammonium chloride were dissolved in 300 ml of deionized water, and then 0.3 mol of phosphoric acid was added thereto under stirring. A 20% aqueous sodium hydroxide solution was added to the solution to adjust the pH to 3.6, and then the resulting precipitates were washed well, and calcined at 900° C. By pulverizing a bulky product obtained by the calcination, a zirconium phosphate compound was synthesized.